(東北大學(xué)有色金屬系冶金物化教研室,沈陽110006)
摘 要: 用化學(xué)鍍法在活性鋁粉表面包覆純鎳層制備Ni-Al復(fù)合粉末。結(jié)果表明,控制溫度為86~89℃、 pH= 12.5~13.2 、硫酸鎳加入量為35.0~45.0 g/ L、還原劑加入量為75~95 mL/ L時可獲得鍍覆質(zhì)量良好的粉末,且鎳呈結(jié)晶態(tài)析出。此外還討論了這些工藝參數(shù)對鍍覆質(zhì)量的影響。
關(guān)鍵字: 化學(xué)鍍 復(fù)合粉末 鍍覆質(zhì)量 工藝條件
BY ELECTROLESS NICKEL PLATING
(Department ofNonferrous Metallurgy,
Northeastern University, Shenyang110006)
Abstract:The composite powders were produced by electroless pure-nickel plating on the surface of activated aluminium powders. The experimental results showed that the well-qualified composite powders can be made by controlling technological parameters and nickel appears in crystal state. The influence of the technological parameters on the coating quality was also given.
Key words: electroless plating composite powders coating quality technological conditions